Where will your fence rust first?
Australia's six corrosion zones, decoded.

A one-page summary of AS/NZS 4534:2006 — Appendix F, the standard Australian engineers, farmers and importers use to choose the right zinc or zinc/aluminium-alloy coating for fencing wire. Use this map to spec the right product for your project — and contact YieldMax for matching coating mass options.

The standard in one paragraph

Australia's outdoor environment can be grouped into corrosivity categories using measured corrosion rates and exposure conditions. The categories help buyers compare how aggressive a site may be when selecting a zinc or zinc-aluminium coating. Local microclimate factors such as salt exposure, rain shielding, fertilisers, galvanic contact, soil and animal waste can materially change performance. Do not apply a universal service-life multiplier without product-specific evidence and site assumptions.

A · Very Low<1.3 µm/y · alpine
B · Low1.3–25 · arid / inland
C · Medium25–50 · coastal cities
D · High50–80 · sea-shore (calm)
E · Very High80–200 · surf / industrial
F · Tropical(≈B) + UV / mould

Australia — measured corrosion sites (Table F2)

A Very Low B Low C Medium D High E Very High F Tropical
WASANT QLDNSWVICTAS Indian Ocean Pacific Ocean Mt Buller (1) Coober Pedy (3) Dubbo (4) Toowoomba (9) Hobart (11) Whyalla (13) Canberra (14) Adelaide (15) Melb-Clayton (18) Perth-Bentley (19) Brisbane (22) Syd-Ryde (22) Geelong (27) Kwinana (29) Sydney (32) Newcastle (35) Altona Bch (35) Pt Kembla (45) Port Pirie (74) Seaford Bch (68) Cowley Bch (142) Newcastle Bch (194) Townsville (15) Tully (20) Innisfail (23) Tropic of Capricorn (≈ Tropical zone above) ⚠ Coastal <1 km strip = D / E

Numbers in brackets are CRMS in µm/year (one-year mild-steel corrosion). Sites overlap on the map where the standard records both city & beach measurements.

Category table (Table F1 + ISO 9223)

CatCRMSISOOutdoor
A<1.3C1Alpine
B1.3–25C2Arid / urban / rural
C25–50C3Coastal
D50–80C4Sea-shore (calm)
E80–200C5Surf / off-shore / industrial
F≈ B—Non-coastal tropics

Corrosivity falls off with distance from the sea

CRMS (µm/y) Distance from coast (km) → 200150100500 01103070100 Surf coast Sheltered bay Arid / inland baseline

Schematic of Figure F1: corrosivity drops sharply within the first ~10 km from a surf coast.

Key concepts to remember

1. The corrosion driver chain

Time of wetnessRH > 80 %, T > 0 °C
+ Airborne pollutantsCl⁻ · SO₂ · H₂S
→ Attack on Zn carbonate barrier
→ Sacrificial Zn loss
→ Steel rusts

2. Microclimate factors that can bump a site to a worse category

a
Initial wet exposure — early rain prevents protective carbonate film from forming.
b
Shielded from rain — salt & fertiliser stay deposited; life cut to ~60 % of rain-washed.
c
Prolonged dampness — bottom fence wires, grass cover, timber posts, bore-water spray.
d
Galvanic contact — Cu, bare steel, stainless or Al within ~1 mm accelerates Zn loss.
e
Soil burial — alkaline clays (e.g. Birdsville) corrode even in Cat B.
f
Chemical contact — CCA timber, lime, fertiliser, fungicide, damp concrete, cinders.
g
Barrier-film abrasion — wind-blown sand, livestock rubbing, wire fretting.
h
Animal enclosures — urine, organic vapours, high humidity.
i
Prevailing winds — SO₂ from power stacks doubles corrosivity up to 80 km away.
j
Fire — Zn melts at 420 °C; coating destroyed near 1000 °C; HT wire softens at 700 °C.

3. Coating life rules of thumb

YieldMax coating recommendation by zone

A practical starting-point spec sheet — confirm against your site's microclimate and the specifying engineer's requirements.

ZoneWhereRecommended YieldMax productTypical coating mass
A · B · FArid, inland, urban, non-coastal tropicsClass 3 heavily galvanised wire / fixed-knot field fence≥ 240 g/m² Zn
CCoastal cities & baysClass 4 galvanised or Zn/5 % Al alloy wire≥ 300 g/m² Zn or ≥ 150 g/m² Zn-Al
DSea-shore, sheltered baysZn/5 % Al alloy ("ZnAl·5") fixed-knot or hinge-joint≥ 215 g/m² Zn-Al
ESurf coast, off-shore, heavy industryZn/5 % Al alloy + PVC sheath where exposed≥ 230 g/m² Zn-Al + PVC

Source: AS/NZS 4534:2006 — Guidance on Corrosion Protection (Appendix F, informative). This summary is provided by YieldMax for planning purposes; the published standard remains the authoritative reference.